Samarium Cobalt Magnets and Magnet Assemblies

IconMagnetic Properties      IconMechanical Properties      IconDemagnetization Curves


Mechanical Properties
Magnet Type Sm-Co 1:5 Sm-Co 2:17
Density g/cm3 8.5 8.4
lbs/in3 0.31 0.3
Compressive Strength MPa 1000 650
psi 1.4x105 0.9x105
Tensile Strength MPa 40 39
psi 6x103 5x103
Bending Strength MPa 120 120
psi 1.7x104 1.7x104
Young's Modulus MPa 110x103 150x103
psi 1.6x107 2.2x107
Stress Crack Resistance KIC(N/mm3/2) 60 45
Electrical Resistance Ω·m 5x10-7 8x10-7
Vickers Hardness Hv 550 600
Curie Temperature °C 750 825
Specific Heat J/(kg·K) 370 390
Coefficient of Thermal Expansion (at 20-100°C) 1/K Perpendicular to c axis 13x10-6 12x10-6
Parallel to c axis 7x10-6 10x10-6

Note: c axis denotes Easy Magnetization Direction (EMD) also called Magnetic Alignment Direction.

Typical Values - not to be used as specifications.
Please contact us at (717) 898-2294 if you need specification values.